High Temperature (HT) Steam Line Repair

Overview

A weld crack was found in a pump room steam line on an FPSO. This line required an in service repair without the use of hot work, met the design temperature of 1830C, and a defect modelled as a circumferential loss of 5mm was required to meet ABS class approval.

The line had the following specifications:

Structure Steam Line
Surface Preparation Sa 2.5
Class Approval ABS
Design Pressure 970 kPa
Design Temperature 1380C
Application Temperature 500C
Design Life 2 years
Wrap Length 1,000 mm
Pipe Diameter 200 mm NB
Corrosion Type Cracking
Defect Details Circumferential through wall
Post Cure Yes - heat tapes

Solution

  • Technowrap™ 2K HT system with temperature capability up to 220°C
  • Heat tapes used to provided post cure temperature of 60°C - 80°C
  • Crack modelled as complete section loss over weld section
  • Sponge-Jet TM surface preparation used for surface preparation

Benefits

  • Sponge-JetTM fully recyclable system reduced equipment and materials footprint led to improve freight costs
  • Start-up design was used to bring line back on line two days quicker
  • ABS approved repair
  • TechnowrapTM provided both structural loads and pressure containing requirements

ICR.IAS JV 

iasgroup is a partner in the ICR.IAS JV, providing leading production critical cold work solutions that remove or minimise the need for shutdowns. The JV is home to market leading technologies TechnowrapTM and QuickflangeTM  https://icrias-jv.com.au/